Rewrite TIG welder page: specs, controls, setup, and shutdown for the PrimeWeld TIG225X
Match control dials to our panel, add ranges and overheat light
 
(One intermediate revision by the same user not shown)
Line 1: Line 1:
<!-- TODO before publishing: confirm which TIG225X version we have. Primeweld's current model adds AC waveform selection and spot welding, which are left out here. Also confirm the outlet and input voltage we use, the torch model fitted, and where tungsten and filler rod are kept. -->
<!-- TODO: add where tungsten and filler rod are kept. Control Dials table confirmed against a photo of our panel (model label TIG225ACDCP), November 2026. -->
== General Information ==
== General Information ==


The PrimeWeld TIG225X is an AC/DC TIG welder with pulse, located in the [[Metal Shop]]. It also does DC stick welding. Use AC for aluminum and DC for steel and stainless steel.
The PrimeWeld TIG225X is an AC/DC TIG welder with pulse, located in the [[Metal Shop]]. It also does DC stick welding. Use AC for aluminum and DC for steel and stainless steel.
Our machine is the 2022–2023 version. It runs on 240V and uses the CK Worldwide 17-series air-cooled torch with Superflex hose that came with it. PrimeWeld's current model adds AC waveform selection and a spot-weld mode; ours does not have them.


Report equipment issues on Slack in #general or #shop-metal.
Report equipment issues on Slack in #general or #shop-metal.
Line 16: Line 18:
|-
|-
| Input
| Input
| 120V or 240V, single-phase
| 240V, single-phase (the machine also accepts 120V, but we run it on 240V)
|-
|-
| TIG output
| TIG output
| 10–225A on 240V; 10–140A on 120V
| 10–225A
|-
|-
| Stick output
| Stick output
Line 25: Line 27:
|-
|-
| Duty cycle (TIG)
| Duty cycle (TIG)
| 40% at maximum output; 100% at 155A on 240V or 108A on 120V
| 40% at 225A
|-
| Torch
| CK Worldwide 17-series, air-cooled, Superflex hose
|-
|-
| Arc start
| Arc start
Line 37: Line 42:
|}
|}


Duty cycle is how much of a 10-minute period the machine can weld at that current. At maximum output, weld for 4 minutes and let it cool for 6. If the machine overheats, its thermal protection stops output until it cools.
Duty cycle is how much of a 10-minute period the machine can weld at that current. At 225A, weld for 4 minutes and let it cool for 6. At lower currents you can weld longer. If the machine overheats, its thermal protection stops output until it cools.


== Orientation and Access ==
== Orientation and Access ==
Line 75: Line 80:


=== Control Dials ===
=== Control Dials ===
These are the dials on our machine's panel, in panel order. The line drawn across the panel between the two rows shows where each setting acts during a weld.


{| class="wikitable"
{| class="wikitable"
|-
|-
! Dial
! Dial
! Range
! Function
! Function
|-
| '''Welding Current'''
| Main amperage. With the foot pedal connected, this sets the maximum the pedal can reach.
|-
| '''Pre-Flow'''
| Gas flow before the arc starts.
|-
|-
| '''Start Current'''
| '''Start Current'''
| 10–225A
| Current when the arc strikes. Lower it for thin sheet metal.
| Current when the arc strikes. Lower it for thin sheet metal.
|-
|-
| '''Up Slope'''
| '''Up Slope'''
| Up to 10 s
| Time to rise from start current to welding current.
| Time to rise from start current to welding current.
|-
|-
| '''Base Current'''
| '''Welding Current'''
| In pulse mode, the low current level, as a percentage of welding current.
| 10–225A
|-
| Main amperage, shown on the AMP display. With the foot pedal connected, this sets the maximum the pedal can reach.
| '''Pulse Frequency'''
| In pulse mode, how many times per second the current switches between peak and base.
|-
| '''Pulse Duty'''
| In pulse mode, how much of each pulse is at peak current. Higher gives more heat and penetration; lower is safer for thin material.
|-
|-
| '''Down Slope'''
| '''Down Slope'''
| 0–25 s
| Time to drop from welding current to end current.
| Time to drop from welding current to end current.
|-
|-
| '''End Current'''
| '''End Current'''
| 10–225A
| Current at the end of the weld, to fill the crater.
| Current at the end of the weld, to fill the crater.
|-
| '''Post Flow'''
| Gas flow after the arc stops. Protects the hot tungsten and weld while they cool.
|-
|-
| '''AC Frequency'''
| '''AC Frequency'''
| 40–200 Hz
| In AC mode, a higher frequency gives a narrower, more focused arc.
| In AC mode, a higher frequency gives a narrower, more focused arc.
|-
|-
| '''AC Balance'''
| '''AC Balance'''
| 10–90%
| In AC mode, the balance between cleaning action, which removes oxide from aluminum, and penetration.
| In AC mode, the balance between cleaning action, which removes oxide from aluminum, and penetration.
|-
| '''Pre-Flow'''
| Up to 3 s
| Gas flow before the arc starts.
|-
| '''Base Current'''
| Up to 95%
| In pulse mode, the low current level, as a percentage of welding current.
|-
| '''Pulses Per Second'''
| Up to 200 Hz
| In pulse mode, how many times per second the current switches between peak and base.
|-
| '''Pulse Duty'''
| From 10%
| In pulse mode, how much of each pulse is at peak current. Higher gives more heat and penetration; lower is safer for thin material.
|-
| '''Post Flow'''
| From 0 s
| Gas flow after the arc stops. Protects the hot tungsten and weld while they cool.
|}
|}
The '''O.C''' light next to the display comes on when the machine overheats or is overloaded. Stop and let it cool before welding again.


== Setup ==
== Setup ==
Line 122: Line 144:
# Make sure the machine is off.
# Make sure the machine is off.
# Set '''TIG / MMA''' to '''TIG'''. Set '''AC / DC''' for your metal.
# Set '''TIG / MMA''' to '''TIG'''. Set '''AC / DC''' for your metal.
# Fit the tungsten. Use a collet and collet body that match the tungsten diameter, and a cup sized for the job. The kit includes 1/16" and 3/32" collets and #5, #6, and #7 cups.
# Fit the tungsten. Use a collet and collet body that match the tungsten diameter, and a cup sized for the job.
# Clamp the ground to clean, bare metal close to the joint.
# Clamp the ground to clean, bare metal close to the joint.
# Open the argon cylinder valve and set the flow on the regulator.
# Open the argon cylinder valve and set the flow on the regulator.
Line 128: Line 150:
# Turn the machine on and set the welding current and post flow.
# Turn the machine on and set the welding current and post flow.


<!-- TODO: argon flow rate, and starting settings for the materials members weld most. -->
== Starting Settings ==
 
These are starting points. Practice on scrap of the same material and thickness, and adjust from there.
 
=== General ===
 
* '''Argon flow:''' 15–20 CFH with a #6 or #7 cup. Use more for larger cups or drafty conditions.
* '''Tungsten:''' 2% ceriated (gray) or 2% lanthanated (blue) works for both AC and DC. Use 3/32" for most work and 1/16" for thin material under about 80A.
* '''Tungsten prep:''' For DC, grind to a point with the grind marks running lengthwise. For AC, grind a point and blunt the tip slightly.
* '''Pre-flow:''' about 0.5 seconds.
* '''Post flow:''' about 1 second per 10A of welding current, and at least 5 seconds.
* '''Pulse:''' off until you are comfortable with standard TIG.
 
=== Steel and Stainless Steel (DC) ===
 
Start at about 1A per 0.001" (thousandth of an inch) of thickness.
 
{| class="wikitable"
|-
! Thickness
! Current
! Tungsten
! Filler rod
|-
| 1/16" (1.6 mm)
| 50–70A
| 1/16"
| 1/16" ER70S-2 (steel) or ER308L (stainless)
|-
| 1/8" (3.2 mm)
| 100–130A
| 3/32"
| 3/32" ER70S-2 (steel) or ER308L (stainless)
|-
| 3/16" (4.8 mm)
| 140–180A
| 3/32"
| 3/32" or 1/8"
|}
 
=== Aluminum (AC) ===
 
Aluminum needs more current than steel of the same thickness, because it conducts heat away quickly.
 
{| class="wikitable"
|-
! Thickness
! Current
! Tungsten
! Filler rod
|-
| 1/16" (1.6 mm)
| 70–100A
| 1/16" or 3/32"
| 1/16" ER4043
|-
| 1/8" (3.2 mm)
| 120–150A
| 3/32"
| 3/32" ER4043
|-
| 3/16" (4.8 mm)
| 170–210A
| 3/32" or 1/8"
| 1/8" ER4043
|}
 
* '''AC balance:''' start with about 30% cleaning (70% penetration). Add cleaning if the puddle looks dirty or peppered. Reduce it if the tungsten balls up or the bead is wide and shallow.
* '''AC frequency:''' about 100–120 Hz for general work. Higher gives a narrower, more focused arc.
* Clean aluminum with a dedicated stainless steel brush and acetone just before welding.
* Near 225A on thick aluminum, watch the duty cycle.


== Shutting Down ==
== Shutting Down ==

Latest revision as of 15:36, 22 November 2026

General Information

The PrimeWeld TIG225X is an AC/DC TIG welder with pulse, located in the Metal Shop. It also does DC stick welding. Use AC for aluminum and DC for steel and stainless steel.

Our machine is the 2022–2023 version. It runs on 240V and uses the CK Worldwide 17-series air-cooled torch with Superflex hose that came with it. PrimeWeld's current model adds AC waveform selection and a spot-weld mode; ours does not have them.

Report equipment issues on Slack in #general or #shop-metal.

PrimeWeld TIG225X in the Metal Shop.

Specifications

Specification Details
Input 240V, single-phase (the machine also accepts 120V, but we run it on 240V)
TIG output 10–225A
Stick output DC stick (MMA)
Duty cycle (TIG) 40% at 225A
Torch CK Worldwide 17-series, air-cooled, Superflex hose
Arc start High-frequency (no-touch) start
Amperage control Front panel or foot pedal
Shielding gas Pure argon

Duty cycle is how much of a 10-minute period the machine can weld at that current. At 225A, weld for 4 minutes and let it cool for 6. At lower currents you can weld longer. If the machine overheats, its thermal protection stops output until it cools.

Orientation and Access

Training is required to use the TIG welder. Complete the general space orientation first. See Welding Equipment for welding orientation, and check the event calendar for upcoming training.

Safety

Follow the Metal Shop safety requirements for helmets, gloves, jackets, ventilation, and flammable materials.

  • The TIG arc gives off strong ultraviolet light. Cover all exposed skin, and close the weld curtain.
  • The tungsten, torch cup, and workpiece stay hot after you stop welding.
  • Clean metal before welding. Do not weld galvanized, plated, or painted metal without removing the coating first.
  • If the tungsten touches the weld pool or filler rod, stop and regrind or replace it. A contaminated tungsten gives an unstable arc.

Controls

Selector Switches

Switch Function
TIG / MMA TIG welding or DC stick welding.
AC / DC In TIG mode: AC for aluminum and magnesium, DC for steel, stainless steel, and most other metals.
2T / 4T 2T: press and hold the torch switch to weld, release to stop. 4T: press to start, release to weld, press again to start the down slope, release to stop. Use 4T for long welds without a foot pedal.
Pulse (Off / Low / High) Off: standard TIG. Low and High set the pulse frequency range.

Control Dials

These are the dials on our machine's panel, in panel order. The line drawn across the panel between the two rows shows where each setting acts during a weld.

Dial Range Function
Start Current 10–225A Current when the arc strikes. Lower it for thin sheet metal.
Up Slope Up to 10 s Time to rise from start current to welding current.
Welding Current 10–225A Main amperage, shown on the AMP display. With the foot pedal connected, this sets the maximum the pedal can reach.
Down Slope 0–25 s Time to drop from welding current to end current.
End Current 10–225A Current at the end of the weld, to fill the crater.
AC Frequency 40–200 Hz In AC mode, a higher frequency gives a narrower, more focused arc.
AC Balance 10–90% In AC mode, the balance between cleaning action, which removes oxide from aluminum, and penetration.
Pre-Flow Up to 3 s Gas flow before the arc starts.
Base Current Up to 95% In pulse mode, the low current level, as a percentage of welding current.
Pulses Per Second Up to 200 Hz In pulse mode, how many times per second the current switches between peak and base.
Pulse Duty From 10% In pulse mode, how much of each pulse is at peak current. Higher gives more heat and penetration; lower is safer for thin material.
Post Flow From 0 s Gas flow after the arc stops. Protects the hot tungsten and weld while they cool.

The O.C light next to the display comes on when the machine overheats or is overloaded. Stop and let it cool before welding again.

Setup

  1. Make sure the machine is off.
  2. Set TIG / MMA to TIG. Set AC / DC for your metal.
  3. Fit the tungsten. Use a collet and collet body that match the tungsten diameter, and a cup sized for the job.
  4. Clamp the ground to clean, bare metal close to the joint.
  5. Open the argon cylinder valve and set the flow on the regulator.
  6. Plug in the foot pedal, or set 2T / 4T to use the torch switch.
  7. Turn the machine on and set the welding current and post flow.

Starting Settings

These are starting points. Practice on scrap of the same material and thickness, and adjust from there.

General

  • Argon flow: 15–20 CFH with a #6 or #7 cup. Use more for larger cups or drafty conditions.
  • Tungsten: 2% ceriated (gray) or 2% lanthanated (blue) works for both AC and DC. Use 3/32" for most work and 1/16" for thin material under about 80A.
  • Tungsten prep: For DC, grind to a point with the grind marks running lengthwise. For AC, grind a point and blunt the tip slightly.
  • Pre-flow: about 0.5 seconds.
  • Post flow: about 1 second per 10A of welding current, and at least 5 seconds.
  • Pulse: off until you are comfortable with standard TIG.

Steel and Stainless Steel (DC)

Start at about 1A per 0.001" (thousandth of an inch) of thickness.

Thickness Current Tungsten Filler rod
1/16" (1.6 mm) 50–70A 1/16" 1/16" ER70S-2 (steel) or ER308L (stainless)
1/8" (3.2 mm) 100–130A 3/32" 3/32" ER70S-2 (steel) or ER308L (stainless)
3/16" (4.8 mm) 140–180A 3/32" 3/32" or 1/8"

Aluminum (AC)

Aluminum needs more current than steel of the same thickness, because it conducts heat away quickly.

Thickness Current Tungsten Filler rod
1/16" (1.6 mm) 70–100A 1/16" or 3/32" 1/16" ER4043
1/8" (3.2 mm) 120–150A 3/32" 3/32" ER4043
3/16" (4.8 mm) 170–210A 3/32" or 1/8" 1/8" ER4043
  • AC balance: start with about 30% cleaning (70% penetration). Add cleaning if the puddle looks dirty or peppered. Reduce it if the tungsten balls up or the bead is wide and shallow.
  • AC frequency: about 100–120 Hz for general work. Higher gives a narrower, more focused arc.
  • Clean aluminum with a dedicated stainless steel brush and acetone just before welding.
  • Near 225A on thick aluminum, watch the duty cycle.

Shutting Down

  1. Let the post flow finish before you lift the torch away.
  2. Turn off the machine.
  3. Close the argon cylinder valve.
  4. Hang the torch and coil the leads. Let the torch cool before storing it.

External Resources